DR.PAX logoAdi Pandžić, PhDEngineering · Design · 3D print Get in touch

Home / Blog

Blog ·

3D-Printed Patterns for Investment Casting: SLA and Clear Cast Resin

In a white paper, Formlabs shows how foundries cast bronze, aluminium, titanium and steel from SLA 3D-printed Clear Cast Resin patterns – without metal tooling for wax patterns and with savings of tens of thousands of dollars.

Investment casting, also known as lost-wax casting, is one of the most versatile foundry processes for producing metal parts with intricate shapes. It is used for lightweight automotive components, golf clubs, jet turbines and art sculptures – wherever a high-quality surface and a high-integrity metal part are required. In the white paper “Industrial Investment Casting With 3D Printed Patterns Using Formlabs Clear Cast Resin”, Formlabs describes how foundries brought SLA (stereolithography) 3D-printed patterns into this process without significant changes to their hardware or workflow.

Key points from the white paper

  • Patterns are printed in Clear Cast Resin, an antimony-free material with very low ash content (below 0.02%).
  • The workflow was validated by the Foundry 4.0 Center at the University of Northern Iowa (UNI) and more than ten foundries – industrial foundries, service bureaus and art foundries.
  • Bronze, brass, aluminium A356, 6-4 titanium, 4140 and 8620 steels, and 316 and 17-4 PH stainless steels were cast.
  • Patterns combine a thin outer wall with an internal lattice and burn out in a furnace at 700–900 °C, with no autoclave.
  • According to Formlabs, foundries reduced tooling costs by up to 90% and cut lead times by several months.
Clear Cast Resin patterns and metal castings: impellers, masks and test parts
Clear Cast Resin patterns and metal castings: impellers, masks and test parts · Image: Formlabs

Where is the bottleneck in traditional investment casting?

Investment casting has three main steps: creating an expendable pattern, building a non-permanent ceramic mould (shell) around it, and pouring liquid metal into the shell. The pattern is traditionally made by wax injection moulding in metal tooling. This requires multiple operations, specialised equipment and extensive skilled labour, and the tooling is usually CNC machined – expensive and slow. As a result, investment casting is particularly costly for low-volume production.

3D printing the sacrificial pattern removes the tooling entirely. According to the white paper, SLA printing puts patterns in hand the next day with very limited equipment, freeing up CNC capacity and skilled operators for other work. SLA delivers the smooth surface finish and high precision that transfer to the final casting, and its design freedom makes complex, intricate patterns possible.

Titanium impellers alongside a Clear Cast Resin pattern
Titanium impellers alongside a Clear Cast Resin pattern · Image: Formlabs

For larger patterns Formlabs offers the Form 4L with a 35.3 × 19.6 × 35 cm build volume, while the Form 4, with 20 × 12.5 × 21 cm, suits smaller parts at high speed.

Case study: aluminium A356 at UNI

The Foundry 4.0 Center at the University of Northern Iowa successfully cast parts in aluminium A356. Parts were converted into a tetrahedron lattice in Materialise's Lattice Module, with 0.5 mm walls and 1 mm lattice diameter. They were printed on a Form 3L at 100-micron layer height, cleaned with the standard Formlabs process and attached to a stock casting sprue with sticky wax.

CAD model of UNI’s impeller pattern with internal lattice
CAD model of UNI’s impeller pattern with internal lattice · Image: Formlabs

The shell used a 100% silica system: Remet RP-1 as the primary coat and RG-1 for backing coats, typically two primary and three backing dips, with stucco applied after the second primary coat and after each subsequent dip. Shelling was fully automated and took 9–10 hours for a single sprue. Once dry, the shell was flash-fired at 900 °C for two hours, preheated to 540 °C, and the aluminium was poured at 700–750 °C. The shell was removed by breaking off the bulk and blasting off the remainder.

What foundries say

John Farr of Diversified Metalsmiths says pattern cost was the main reason for buying the Form 3L. For one impeller they started with the customer's wax injection tooling, then moved to PMMA printed patterns whose price rose to over $300. Even amortising the printer and equipment, they expect at least to break even on the current order and to save more than $200 per part on upcoming orders, with very little difference in the process before and after casting.

Julian Mussi of Thesis Digital Arts notes that Clear Cast lets them produce highly detailed patterns for art casting faster, more consistently and at a fraction of the labour cost of hand-chased wax patterns.

Mask printed in Clear Cast Resin and the final metal casting
Mask printed in Clear Cast Resin and the final metal casting · Image: Formlabs

Results and cost analysis

Based on user feedback, Clear Cast Resin patterns produce castings of quality comparable to traditional wax patterns. Printed patterns may be more brittle than wax and should be handled with care, but burnout is clean with no noticeable ash in the visible part of the shell, and the final metal part shows no unusual defects. Undercuts, tortuous channels and thin walls that are hard to achieve with wax injection are easy to print – without tooling, soluble cores or other complex wax techniques.

Savings in the white paper examples
PartComplex impellerSimple pump impeller (12″)
Production volume50 parts50 parts
Alternative methodWax injection with metal tooling, soluble wax cores and wax chillsWax injection with metal tooling
Alternative tooling cost$60,000$11,000
Printed pattern cost$78 per part$30 per part
Lead time saved14 weeks8 weeks
Latticed printed patterns and the cast metal parts
Latticed printed patterns and the cast metal parts · Image: Formlabs

The eight-step workflow

The white paper provides a guide based on feedback from more than ten foundries: 1. pattern design, 2. pattern 3D printing, 3. pattern preparation, 4. shell making, 5. pattern burnout, 6. metal pouring, 7. shell removal and 8. cutting off and finishing.

1. Designing a latticed pattern

A sacrificial pattern must withstand the pressure of the ceramic slurry while being thin enough to burn away with as little ash as possible. It therefore combines thin outer walls with a strong internal lattice. The part is designed in any CAD software, then hollowed and latticed in a tool such as Materialise Magics.

Internal lattice of a casting pattern in Materialise Magics
Internal lattice of a casting pattern in Materialise Magics · Image: Formlabs
Recommended lattice settings (mm)
SettingValue [min/max]
Wall thickness0.5 [0.4/1]
Detail size0.5
Leg thickness (a)0.75 [0.5/1]
Leg length (b)3
Radius outer circle (r2)2
Radius inner circle (r1)2

Thinner walls increase casting success but reduce print success and weaken the part, so Formlabs suggests starting at 0.5 mm and increasing only after print failures or accuracy problems. Thicker lattice legs reinforce the pattern but raise the risk that it expands and cracks the shell – 0.75 mm is the recommended start.

Drain and vent holes reduce the risk of “suction cup” and “explosion” print failures and let trapped liquid resin drain. Place them at the top and bottom of the print orientation, preferably on sacrificial surfaces, with at least a 1 mm radius, straight or only slightly chamfered, and put a vent where the sprue will attach to aid airflow during burnout. Because latticed files are large, exporting to 3MF is recommended.

2. 3D printing the pattern

In PreForm the model is oriented 30–45° to the build platform, with the vent holes in mind. Add a full raft and light supports at 0.75 density with 0.30 mm touch tips or smaller, away from critical surfaces. Print on Form 4L, Form 3L or Form 4 at 100-micron layer height.

UNI’s patterns on the Form 3L build platform
UNI’s patterns on the Form 3L build platform · Image: Formlabs

Wash the part in Form Wash L in IPA for 10 minutes, blow out the interior with compressed air, then wash for another 5 minutes. Removing all trapped IPA is critical, as any remaining liquid can vaporise during burnout and crack the shell. Post-cure for 15 minutes at 35 °C in Form Cure L, or without heat if the part is prone to warping. Supports come off more easily before curing, but removing them afterwards is safer for fragile geometries; use scrapers, flat snips or 100–300 grit sandpaper.

3. Preparing the pattern

Fill the vent and drain holes with standard foundry wax or a UV resin pen cured for about 30 seconds, and check for leaks by forcing compressed air into the last hole. Then assemble as usual: attach the pattern to a wax tree with adhesive wax and add a T-bar for dipping. The sprue can also be printed as part of the pattern. Some foundries add vents to improve airflow in burnout, which is recommended for one-offs and time-sensitive deliveries.

4. Shell making

Foundries can keep their usual slurry dipping process; Formlabs has seen no shell-adhesion problems with printed patterns. For reference, UNI uses a robotic cell with six dips: one primary slurry dip without sand to preserve surface finish, one backing slurry dip with primary sand and three backing dips with backing sand to build thickness and strength, and a final primary dip without sand as a seal coat.

UNI’s robotic cell dipping the tree in the primary slurry
UNI’s robotic cell dipping the tree in the primary slurry · Image: Formlabs

5. Pattern burnout

Flash firing is the standard method, heating the pattern to 705–900 °C for two hours. A foundry needs a high-temperature furnace and sufficient oxygen flow. In an autoclave, or below 650 °C, patterns are likely to crack the shell. After burnout, check the shell for cracks or flashing and blow out any remaining ash. Clear Cast Resin contains under 0.020% ash by mass and is printed hollow, so only a trivial amount remains.

UNI’s burnout furnace
UNI’s burnout furnace · Image: Formlabs
Tree during flash firing in the furnace
Tree during flash firing in the furnace · Image: Formlabs

6–8. Casting, shell removal and finishing

Casting and finishing follow the foundry's usual process. UNI preheats the shell in a kiln at 345 °C for 30 minutes, pours the metal and lets it solidify completely. The ceramic shell is removed with a water or sand blaster – chiselling should be avoided where possible to protect the part – and the parts are separated from the tree with a bandsaw or other tools.

Ceramic shell cooling after the metal pour
Ceramic shell cooling after the metal pour · Image: Formlabs

How the materials were tested

In the appendix, UNI compared a beta version of Clear Cast Resin, BioMed Clear Resin and a popular competitor resin. Tests covered compression strength, flexural strength, ash content and thermal expansion, and Formlabs additionally measured trace elements.

Compression strength. 58 samples were tested in nine geometries with different wall (0.5–1 mm) and leg (0.5–1 mm) thicknesses. Beta Clear Cast was stronger than the competitor process at geometry B, but its strength dropped sharply with a small change in wall thickness. Because the printers' low forces and high accuracy maintain quality at thinner geometries, a thinner geometry was selected – lower crush strength means less stress on the shell.

Average compression strength for each sample geometry and resin
Average compression strength for each sample geometry and resin · Chart: Formlabs / UNI

Flexural strength. Four samples of each material were tested to ASTM D790. Both Formlabs materials showed higher flexural strength, meaning patterns that better survive rough handling in the foundry.

Flexural strength to ASTM D790 (ksi)
Flexural strength to ASTM D790 (ksi) · Chart: Formlabs / UNI

Ash and trace elements. Tested to ASTM D2584, beta Clear Cast had 0.024% ash and BioMed Clear 0.006%. Elemental analysis of beta Clear Cast found antimony below 10 ppm, aluminium and copper above 10 ppm, no transition metals above 50 ppm, and tin, silicon and phosphorus above 10 ppm, noting some batch-to-batch variation.

Thermal expansion. Dilatometer results showed that thermal expansion was the key issue with BioMed Clear, while beta Clear Cast had a lower final expansion than the competitor resin, making shell cracking less likely. Casting trials confirmed this: Clear Cast was cast many times without damaging the shell, whereas some BioMed Clear patterns cracked it.

Thermal expansion measured with a dilatometer
Thermal expansion measured with a dilatometer · Chart: Formlabs / UNI

Why this matters for engineers and foundries

The white paper concludes that 3D-printed patterns lower costs and lead times for rapid prototyping, quick-turn orders and limited production runs. As a toolless method, it lets foundries respond faster to customers, delay investment in hard tooling and validate designs cost-effectively. For engineers, it means design for additive manufacturing (DfAM) and design-for-casting rules can be combined at the CAD stage – from wall and lattice thickness to the placement of holes and sprues.

Checking the dimensions of a cast part with a caliper
Checking the dimensions of a cast part with a caliper · Image: Formlabs

You can read the full document on the Formlabs website. If you need a part designed for 3D printing or casting, see my 3D printing services and product design.

About the source
SourceFormlabs white paper
Original titleIndustrial Investment Casting With 3D Printed Patterns Using Formlabs Clear Cast Resin
Publication dateSeptember 5, 2024 (released with Clear Cast Resin)
Testing partnersFoundry 4.0 Center, University of Northern Iowa, and more than ten foundries

Frequently asked questions

Can a 3D-printed pattern replace a wax pattern in investment casting?

According to the Formlabs white paper, Clear Cast Resin patterns produce castings of quality comparable to wax patterns, with a clean burnout and no unusual defects in the metal part. The printed patterns are more brittle than wax, so they should be handled with care.

Which metals were cast with Clear Cast Resin patterns?

Partner foundries cast bronze, brass, aluminium A356, 6-4 titanium, 4140 and 8620 steels, and 316 and 17-4 PH stainless steels.

Why does a 3D-printed casting pattern have an internal lattice?

A thin outer wall with a lattice inside gives enough strength for dipping in ceramic slurry while leaving little material to burn out. That means less ash and less expansion that could crack the shell.

How much can be saved compared with metal tooling?

In the white paper's examples, tooling for a complex impeller would cost $60,000, while a printed pattern cost $78 per part with a 14-week shorter lead time. Formlabs reports that foundries cut tooling costs by up to 90%.

This article summarises a white paper published by Formlabs; please refer to the original document for details and exact data. About the author

← All articles